Diamond wire cutting for optical glass, 石英ガラス, borosilicate and display glass — where the requirement is a cut that can go straight to lapping without a grinding step.
The requirement is different from other materials
Cutting optical glass is not about removing material quickly. It is about leaving a surface that the next process can fix. A wire cut that produces 30 µm of subsurface damage costs more in lapping time than it saved in cutting time. The target is usually damage depth below 20 µm and no edge chip larger than 0.1 ミリメートル.
Wire and slurry choices
| Glass type | Wire Ø | Abrasive | Feed | Character |
|---|---|---|---|---|
| Fused silica / 石英 | 0.20–0.35 mm | D30–D64 | 0.2–0.5 mm/min | Brittle, chips at edges |
| Borosilicate | 0.25–0.45 mm | D64–D126 | 0.4–1.0 mm/min | Forgiving, good for trial cuts |
| Display / float glass | 0.30–0.50 mm | D126 | 0.8–2.0 mm/min | Thin stock, support is critical |
| Chalcogenide / soft optical | 0.20–0.30 mm | D30 | 0.1–0.3 mm/min | Thermally sensitive, cold coolant |
Why glass cuts fail
Glass has no plastic zone, so there is no warning before failure. Three mechanisms account for nearly all losses:
- Edge chipping at breakthrough — the wire exits into air and the last few millimetres are unsupported. Sacrificial backing plates solve this; slower feed only postpones it.
- Thermal cracking — glass conducts heat poorly, so the kerf heats locally. Coolant must reach the kerf, not just the part.
- Wire wander on thin stock — below 1 mm thickness the wire has nothing to guide it. Reduce guide spacing rather than reducing feed.
Getting from cut to polish
The cut face should be flat enough that lapping starts with a coarse but not aggressive step. A good wire cut on borosilicate typically allows starting lapping at 9 µm rather than 30 µm — that is two process steps removed from the route, which is where the real cost saving sits.
Frequently asked questions
Can diamond wire cut tempered glass?
いいえ. Tempered glass releases its stress field when the cut penetrates the tension layer and shatters. It must be cut before tempering, or cut by a process that removes the temper first.
Is laser cutting better for thin glass?
For very thin stock and for internal features, often yes. For thick sections, for stacked plates and for anything where edge quality at depth matters, wire is more predictable and cheaper per part.
What determines the damage depth?
Mostly abrasive grit size and feed per revolution, in that order. Halving grit size roughly halves damage depth; halving feed gets you about a third of the improvement.